From: Comparison of teak wood properties according to forest management: short versus long rotation
Long rotation teak | Short rotation teak | |
---|---|---|
Dichloromethane extractive content (%) | 2.8 ± 0.10 | 0.5 ± 0.06 |
Acetone extractive content (%) | 1.1 ± 0.28 | 0.3 ± 0.05 |
Toluene/ethanol (2/1) extractive content (%) | 1.6 ± 0.15 | 0.4 ± 0.06 |
Water extractive content (%) | 2.5 ± 0.45 | 2.5 ± 0.48 |
Total extractive content (%) | 8.0 ± 1.55 | 3.7 ± 0.85 |
Holocellulose (%) | 68.53 ± 0.63 | 67.50 ± 1.53 |
Cellulose (%) | 49.18 ± 0.60 | 48.80 ± 1.19 |
Hemicellulose (%) | 19.35 ± 0.92 | 18.70 ± 1.72 |
Lignin (%) | 32.19 ± 0.76 | 35.53 ± 0.78 |