Table 4 MC and mechanical properties obtained by four-point bending test on dry logs

From: Use of non-destructive test methods on Irish hardwood standing trees and small-diameter round timber for prediction of mechanical properties

Species

Thinning

MC

MOEm

fm

Density

Mean (%)

COV (%)

Mean (N mm−2)

COV (%)

Mean (N mm−2)

COV (%)

Mean (kg m−3)

COV (%)

Alder

1st

12.6

5.2

5735

10.5

61.83

16.8

498

7.1

2nd

15.1

10.4

7740

11.9

51.79

24.4

481

4.6

Both

13.8

12.5

6738

18.8

56.81

22.2

489

6.3

Ash

1st

18.2

8.1

10162

16.9

65.11

11.1

668

6.9

2nd

18.4

9.4

9435

12.6

60.86

11.5

659

7.3

Both

18.3

8.8

9799

15.5

62.99

11.8

664

7.2

Birch

1st

19.8

10.1

8076

13.8

47.33

18.9

592

3.9

2nd

18.8

9.6

7519

13.2

49.75

14.3

606

2.1

Both

19.3

10.2

7797

14.0

48.54

16.9

599

3.3

Sycamore

1st

10.3

8.0

6391

22.0

43.90

13.9

560

5.1

2nd

14.4

9.9

8918

12.0

56.02

11.5

542

8.3

Both

11.9

19.1

7339

24.2

48.45

17.7

553

6.6

All together

16.0

22.2

7949

23.1

54.50

20.7

578

12.8