Table 5 Colour parameters measured in logs of Hieronyma alchorneoides from the fast-growth plantation under different treatments and different tree heights

From: Reduction of growth stresses in logs of Hieronyma alchorneoides Allemão from fast-growth plantations using steaming and heating: effects on the quality of lumber

Tree height (m)

Treatment

Colour parameters in the heartwood

Colour parameters in sapwood

L*

a*

b*

L*

a*

b*

0.0–2.5

Untreated

23.2B (22.3)

13.6C (39.8)

9.3B (57.9)

52.1B (13.8)

20.3A (20.3)

26.1A (16.5)

Heatingtreatment

39.2A (23.7)

16.7B (23.5)

16.8A (26.1)

63.2A (5.4)

13.1B (17.1)

22.8B (7.1)

Steamingtreatment

36.8A (18.2)

20.0A (23.8)

17.0A (22.1)

61.1A (8.1)

14.0B (16.5)

21.5B (12.3)

2.5–5.0

Untreated

22.4B (24.8)

13.7C (40.4)

8.9C (54.4)

53.1C (14.8)

19.6A (25.9)

25.2A (24.3)

Heatingtreatment

36.4A (20.9)

17.4B (10.9)

16.3B (22.0)

64.1A (8.8)

11.3C (20.2)

22.1B (6.0)

Steamingtreatment

37.1A (12.9)

20.0A (13.3)

19.8A (19.9)

58.3B (9.8.7)

15.7B (19.0)

23.0AB (12.9)

5.0–7.5

Untreated

29.8B (32.3)

18.8A (20.8)

12.8B (35.6)

62.2A (10.0)

15.5A (28.7)

25.3A (23.0)

Heatingtreatment

45.0A (8.7)

20.7A (12.0)

22.5A (16.4)

65.0A (5.0)

12.2B (17.2)

22.9A (7.4)

Steamingtreatment

43.4A (9.5)

20.9A (10.4)

20.5A (12.8)

63.2A (4.4)

13.6AB (15.3)

22.6A (8.2)

7.5–10.0

Untreated

66.3A (4.9)

12.4A (20.8)

23.2A (29.6)

Heatingtreatment

38.9A (30.0)

17.1B (9.2)

15.9B (30.1)

63.7AB (6.0)

12.3A (29.2)

22.5A (9.5)

Steamingtreatment

47.9A (3.6)

22.1A (14.3)

34.3A (51.7)

60.1B (4.7)

14.8A (12.0)

21.7A (9.8)

  1. The values in parentheses correspond to the coefficients of variation. Different letters between treatments mean there are statistical differences (P < 0.05)